Easy Solar Dyeing with bought Cherry Juice

Solar Dyeing with Cherry Juice


This is basically putting your dyestuff in a glass jar and leaving it in the sun to work its magic. The beauty of living in Australia means that I do have the benefit of hot summers. If you don’t have these conditions, it does not mean you cannot try this process. You will just need to experiment with your own environments advantages and disadvantages. Leave it in a room that gets sunlight and may have great heating or try longer dyeing periods.

In this particular experiment we will actually look at longer dyeing periods with Cherry Juice. Even in a hot Australian summer, some dye material needs a longer time frame than others.

The procedure that I have used below is only 1 example of how to dye with juice. These experiments are only to show you what has and hasn’t worked for me, so you can pick through the information to start your own experimenting journey.

Safety Note

Always ensure when dyeing of any nature, to keep all saucepans and utensils used in the process, separate from your general cooking supplies. You do not want to cook with anything that has been used to mordant or naturally dye your fibres. You should also wear gloves and a mask while handling your chemicals.

Washing your Wool


The main thing to avoid while washing your fibre, is to not make any sudden temperature changes. Putting your wool in a hot tub, will start the felting process, and make your fibre shrink and clump together.

You should also take care not to agitate your fibre in the water too much. This will also start the felting process. Always make sure you use gentle squeezing motions while cleaning.

When washing your fibre both before or after the dyeing process, you should always use a gentle soap. You do not want a harsh detergent that will leave chemicals, that will later wash out your dye. Something like olive oil or goats milk soap will work effectively, while being much gentler on your fabric.

I personally don’t use heat while washing my wool or silk, and so far have had no problems with dyeing. Everybody’s wool however may be different and have different things added during processing , so if you are getting streaky results in your dyeing, try putting your fibre and detergent in a pot for half an hour. Keep the water temperature at a simmer. This will replace the second stage of the process below. Do not let the water boil.

Step 1: Soak bath

We need to soak the fibre first, before we do anything else. This will help the cells to open up and be receptive to the washing up detergent.

Fill a large bowl or saucepan with room temperature water, making sure that the fibre will not go through any sudden temperature changes. Make sure there is enough room for the fibre to move freely.

Add your fibre gently into the water. If you are washing wool, you may need to gently squeeze the air out of the fibres (while underwater) to stop it from floating on the surface.

Leave for at least 15 min.

Step 2: Wash Bath

Take your fibre out ( gently squeezing the excess water) and make another bath as above. This time add some gentle soap to the bath, before placing your fibre back in.

Leave for at least 30min though preferably longer.

Step 3: Rinse Bath

Take your fibre out ( gently squeezing the excess water out) and repeat step 1, allowing it to rest for at least 30 min. You can give the fibre a few gentle squeezes to help get the soap suds out. If your fibre still looks soapy you can give it an extra rinse bath until it looks clean and clear.

After washing your fibre you can move straight on to mordanting or leave to dry for a later date.

Mordanting your Wool with Alum


Measurements.

The first thing you will need to do is weigh your fibre. You will need to know how much fibre you have, to determine how much alum and cream of tartar to use in your solution. This measurement is called WOF (weight of fibre). You should always weigh you fibres when dry and free from debris.

In most instances I use 10% WOF of alum and 7% WOF of cream of tartar. Different recipes can use different amounts of alum. but unless otherwise stated, you can safely assume I have mordanted my fibres with 10%. I would not recommend going above 15% of alum, as it may deteriorate you fibres in the long run.

So if you have 100g of fibre, you will need 10g of alum and 7g of cream of tartar.

Weigh these out and dissolve them in hot tap water first.

Process

Step 1:

Place enough water in your saucepan so your fibres can move freely. The water needs to be able to easily move around and through your fabric/fibre to fully get the chemicals to penetrate.

Step2:

After weighing our fabric / fibre and calculating how much Alum and Cream of Tartar you need, dissolve them in a glass of hot tap water. You need to give them a good stir to get all of the granules dissolved. Add your dissolved chemicals into the water and stir.

Step3:

Gently add your wet fibres and submerge them under the water. You may need to gently squeeze your fibre to release air bubbles. Any air traps in the fibre will block the mordant from attaching to it. While doing this, be as gently as possible if you are mordanting wool. You do not want to agitate the wool too much as it may cause it to felt. Take your pot to the stove. Place a thermometer into the pan.

Step 4:

Turn your stove top on and allow the water to get to 80 degrees Celsius (176 Fahrenheit).

Step 5:

Leave your fibre for 40 min at 80 degrees. Do not allow your water to boil! If you are mordanting wool it will start felting when in boiling water.

Step 6.

Turn your heat off and leave the pan on the stove top to cool down. You want your fibre to cool down gradually.

I normally leave the fibre in the saucepan overnight for a bit of extra time in the mordant. You can however take it out as soon as it has cooled down to begin the dyeing process.

You can now move on to dyeing your fibre with cherry juice or let it dry before putting it away for future use. If you do let it dry for later, make sure to let it stand in some water again before dyeing. Your fibres will attract the dye much easier if they are wet.

I always try to mordant as big a batch of fibre as my saucepan will comfortably fit. You can then hang it out to dry and re wet when you are ready to dye. I find it much more economical and quicker to batch scour and mordant my fibres.

If you are re wetting your mordanted fibres for dyeing, leave them in the water for at least 15 minutes. This allows the cells in your fibre to open up and accept the natural dye much easier. This is the same if you have washed fibre that has been dried and needs to be re wetted before mordanting. As with the earlier processes, you will need to gently place the fibre in room temperature water and gently squeeze out any air bubbles. You do not want to agitate the wool too much as it may cause it to felt.

dyeing with cherry juice

Dyeing your Wool with Cherry Juice


For this experiment I used 3 dye baths. 2 that would be left for 1 week, and the other left for 4 weeks.

What You will Need

Cherry Juice- Check that your Cherry juice is 100% natural. You do not want any additives or chemicals changing your results. I was not able to get fresh juice, it was reconstituted, but there were no additives so it was the best I could do.

The amounts used are not subject to any great formula of dye stuff to fabric. For this particular experiment I just used a 1 litre bottle of juice for each. Give whatever you have on hand a go!

Wool Fibre- In this instance I have used 10g of Merino wool roving and 20g of Finn wool roving, mordanted with alum.

Glass Jar- I used 3 for this experiment, 1 for each dye bath. Your glass jars should be big enough for your dye bath to move around your fibre easily and gently. A 1 litre jar is about the smallest I would go for 10g of roving.

dyeing with cherry juice

Procedure

Step 1: Place your cherry juice into the jar. Add your fibre . I set up 3 jars. In 1 I placed 10g of Merino roving and in the other 2, 10 g of Finn roving each.

I left the Merino roving and 1 of the Finn roving jars in the sun for 1 week. The other Finn jar was left for 4 weeks. (It was summer in Australia, so was quite warm)

Step 4: Take your wool out of the jar and leave to dry completely without rinsing.

Step 5: Rinse in water baths until they are clear. As I was using roving I did not want to use running water to start it felting, so I used a few bowls of water. Always make sure you wool does not experience dramatic temperature changes as this can start the process of felting your wool. Make your water room temperature. For the same reason you do not want to agitate your wool too much. Use gentle movements at all times. Leave to dry

Results for dyeing with cherry juice


As you can see in the pictures we started off with some pale pink/beige and ended with a much more striking colour

The first pictures are of the 1 week experiments and show the initial dyed roving after it has been rinsed and dried. I have then turned the roving into felt using a wet felting process. It seems that the wet felting procedure would be a good indication of how well the dye stands up to washing as it gets vigorous applications of soap and hot water.

The felt was then left on a window sill for 4 weeks for a sun test. This is the 3rd circle in each picture. As you can see there has been a very slight fading but considering this was the middle of a hot Aussie summer, it really was quite negligible.

Dyeing with cherry juice has really been quite successful. There was not a lot of difference between the 2 different breeds of wool, but the difference between 1 week and 4 weeks in the dye bath really did matter for this one.

dyeing with cherry juice

Update 8/8/2024


I have since done some additional cherry juice dyeing on 2 ply thread merino wool. These wools were dyed for 4 weeks using the solar dyeing method. The threads dyed a little different in colour as the roving. The colour was not as orange.

The first picture shows the results of the sun test, with the dye standing up very well to the hot aussie sun.

The second picture shows a wash test. The first square is the tread while it is still wet from spraying water onto it. The second shows the same embroidery after it has been hand washed with a gentle soap and warm water. I was really happy to see no bleeding of colour happening at all.

I hope this helps and encourages you to try your own experimenting in the world of natural dyes. 🙂